Espelund Experiment A - April 30, 2008

Production of iron rich slag only - Norse short shaft furnace.
CLOCK ELAPSED EVENT AIR CHARCOAL   ORE    
        COUNT TOTAL COUNT AMOUNT TOTAL
          kg 500 gm kg kg
                 
12:14   start wood splints pre-heat            
12:23   partial lid over furnace top            
13:45   fill with wrist thick pieces            
13:53     gentle          
13:55   block tap arch with sod            
14:06   first addition rough charcoal 120 2.5 2.5      
14:11   second amount rough charcoal   2.5 5      
14:19   fill to 30 cm above tuyere   7.5 12.5      
14:31 2:17 start main sequence            
                 
14:31   adjust air 150          
14:37 0:06 burn to top of charcoal   1 1      
14:49 0:12     1 2      
14:57 0:08     1 3      
15:07 0:10   175 1 4      
15:16 0:09   200 1 5      
15:25 0:09   full 1 6      
15:36 0:11     1 7      
15:37   added as single slug       2 1 1
15:42   added as single slug       2 1 2
15:46 0:10     1 8      
15:49           2 1 3
15:52           2 1 4
15:57 0:11     1 9      
16:00           2 1 5
16:06           2 1 6
16:09 0:12     1 10      
16:13           2 1 7
16:16           2 1 8
16:17 0:08     1 11      
16:26           4 2 10
16:28 0:11     1 12      
16:30           2 1 11
16:36           2 1 12
16:39 0:11     1 13      
16:40           2 1 13
16:49 0:10     1 14      
16:57 0:08 start burn down   1 15      
                 
                 
2:26   TOTALS     15     13
                 
    Main Slag mass 7.5          
    Slag fragments 3.7          
    SLAG PRODUCED 11.2          
    return 86%          

Last Updated on 6/10/08
By Darrell Markewitz